Guizhou Zimuyu Gold Mine Heap Leaching Example

Nature of the ore to ore produced on weathered rock oxide interface, of the strong mud, red red brown iron mineralization, or quartz particles having a quartz vein. It is soft and has a moisture content of up to 26%. The main gangue minerals are kaolinite, hydromica , quartz, limonite, accounting for 96.3%-97.1%, gold particle size is 4.3-5.0μm, which is fine-grained gold; wrapped in iron dolomite, vulcanized The gold content is 2.3% to 3.8%, and the chemical composition of the ore is as follows (see Table 1):

Table 1

SiO 2

Fe 3 +

Al 2 O 3

TiO 2

P

CaO

MgO

S

As

Cu

Zn

Sb

53.19

10.49

16.73

3.44

0.148

0.16

0.55

0.027

0.44

0.024

0.015

0.008

Heap leaching Because the local coal resources are abundant, the price is cheap, and the pit is used for drying. After drying, the ore moisture content is reduced from 26% to less than 15%. After adding 10 kg of cement per ton of ore, 20 kg of lime, the ore, The cement and the lime are mixed and transported to the crusher by a belt. After being crushed, the belt is sent to a pan granulator for granulation. At the time of granulation, a previously prepared granulation liquid having a composition of 0.5% sodium cyanide and 1 × 10 -5 of a scale inhibitor was added. The residence time of the control pellets in the tray is 6-12 min. The pellet moisture is between 24% and 26%. After curing for 24 hours, pile up, the stack height is 2.5 ~ 3.0m, and the angle of repose is 45 °. Using PLK-15 rotating nozzle cloth liquid, the spray intensity is 15L/(h·m 2 ), the gold in the leachate is adsorbed by the carbon column, the gold-loaded carbon is sent to the desorption electrolysis center, and the gold mud is fused to obtain the combined gold, and the color is up to 98. %the above.

The final result: the original ore grade is 2.49~5.3g∕t, the slag grade is 0.17~0.28g∕t, the leaching time is 15~19d, and the leaching rate is over 93%. The recovery rate is 86.87% to 87.97%.

Waste treatment After the leaching is completed, the heap is washed with water and then sprayed with calcium hypochlorite solution until the cyanide concentration of the effluent from the heap is less than 0.5 mg ,L, and the tail slag is finally sent to the tailings dump. The final discharge of the wastewater is also treated with a calcium hypochlorite solution until the cyanide concentration is less than 0.05 mg ∕L.

Table 2 shows the granulation heap leaching indicators for some mines in China.

Table 2 Domestic granulation heap leaching indicators

Mine name

Ore nature

Metal grade

Adhesive addition amount (kg∕t mine)

Agglomerate water content (%)

Leaching cycle (d)

Metal recovery rate (%)

lime

cement

Zimuyu Gold Mine

Clay mine

Au 2.49g∕t

15

0.8

26

19

87.97

Muping phosphorus fertilizer plant

Pyrite cinder

Au 2.69g∕t

-

2.0

20

38

69.76

Langquan Gold Mine

Silicified slate mud

Au 2.54g∕t

0.7

1.0

20

42

67.4

Longwangshan Gold Mine

Iron cap type oxidized ore

Au 4.76g∕t

1.0

0.54

12.5~15

75

71.8

Guangxi uranium mine

Uranium and molybdenum off- balance

U 0.089%

2.0

13

90

U 43.82

Mo 0.163%

Mo 58.28

Yunnan uranium mine

Argillaceous sandstone

U 0.145%

N603 0.04%

12

9~12

>90

Jinchuan Nickel Mine*

Off-balance sheet mine

Ni 0.4%

N603 0.1%

15

35

Ni 82

Cu 0.26%

Cu 65

Co 0.018%

Co 78

* Indoor column immersion test results.

Double Corrugated Roll Forming Machine: Two layers all make corrugated panel, it can be different parameters, rollers and width of materials. IBR roll forming machine or water wave color steel panel making machine is our factory`s main products. The up layer and down layer can be different rollers according to the different model of panel. Arc type roll forming machine.

Double Corrugated Roll Forming Machine

Double Corrugated Roll Forming Machine

Corrugated Double Deck Forming Machine,Water Wave Double Deck Roofing Making Machine,Corrugated Roll Forming Machine ,Corrugated Sheet Roll Forming Machine

Xianfa Roll Forming Machine Factory , https://www.btxianfa.com